This MedLibrary.org supplementary page on Magnetic susceptibility is provided directly from the open source Wikipedia as a service to our readers. Please see the note below on authorship of this content, as well as the Wikipedia usage guidelines. To search for other content from our encyclopedia supplement, please use the form below:
Related Sponsors
In electromagnetism the magnetic susceptibility (latin: susceptibilis “receptiveness”) is the degree of magnetization of a material in response to an applied magnetic field.
Definition of volume susceptibility
-
- See also Relative permeability.
The volume magnetic susceptibility, represented by the symbol
(often simply
, sometimes
— magnetic, to distinguish from the electric susceptibility), is defined by the relationship
where, in SI units,
- M is the magnetization of the material (the magnetic dipole moment per unit volume), measured in amperes per meter, and
- H is the magnetic field strength, also measured in amperes per meter.
The magnetic induction B is related to H by the relationship
where μ0 is the magnetic constant (see table of physical constants), and
is the relative permeability of the material. The magnetic susceptibility χv and the magnetic permeability μ are related by the following formula:
.
Sometimes [1] an auxiliary quantity, called intensity of magnetization and measured in tesla, is defined as
.
This allows an alternative description of all magnetization phenomena in terms of the quantities I and B, as opposed to the commonly used M and H.
Conversion between SI and cgs units
Note that these definitions are according to SI conventions. However, many tables of magnetic susceptibility give cgs values (often denoted by "emu" or "e.m.u.", short for electromagnetic unit) that rely on a different definition of the permeability of free space:[2]
The dimensionless cgs value of volume susceptibility is multiplied by 4π to give the dimensionless SI volume susceptibility value:[2]
For example, the cgs volume magnetic susceptibility of water at 20°C is −7.19×10−7 which is −9.04×10−6 using the SI convention.
Mass susceptibility and molar susceptibility
There are two other measures of susceptibility, the mass magnetic susceptibility (χmass or χg, sometimes χm), measured in m3·kg−1 in SI or in cm3·g−1 in cgs and the molar magnetic susceptibility (χmol) measured in m3·mol−1 (SI) or cm3·mol−1 (cgs) that are defined below, where ρ is the density in kg·m−3 (SI) or g·cm−3 (cgs) and M is molar mass in kg·mol−1 (SI) or g·mol−1 (cgs).
- χmass = χv / ρ
- χmol = Mχmass = Mχv / ρ
Sign of susceptibility: diamagnetics and other types of magnetism
If χ is positive, then (1+χv) > 1 (or, in cgs units, (1+4πχv) > 1) and the material can be paramagnetic, ferromagnetic, ferrimagnetic, or antiferromagnetic. In this case, the magnetic field is strengthened by the presence of the material. Alternatively, if χ is negative, then (1+χv) < 1 (or, in cgs units, (1+4πχv) < 1), and the material is diamagnetic. As a result, the magnetic field is weakened in the presence of the material.
Experimental methods to determine susceptibility
Volume magnetic susceptibility is measured by the force change felt upon the application of a magnetic field gradient [3]. Early measurements were made using the Gouy balance where a sample is hung between the poles of an electromagnet. The change in weight when the electromagnet is turned on is proportional to the susceptibility. Today, high-end measurement systems use a superconductive magnet. An alternative is to measure the force change on a strong compact magnet upon insertion of the sample. This system, widely used today, is called the Evan's balance.[4] For liquid samples, the susceptibility can be measured from the dependence of the NMR frequency of the sample on its shape or orientation[5][6][7][8][9].
Tensor susceptibility
The magnetic susceptibility of most crystals is not a scalar. Magnetic response M is dependent upon the orientation of the sample and can occur in directions other than that of the applied field H. In these cases, volume susceptibility is defined as a tensor
- Mi = χijHj
where i and j refer to the directions (e.g., x, y and z in Cartesian coordinates) of the applied field and magnetization, respectively. The tensor is thus rank 2, dimension (3,3) describing the component of magnetization in the i-th direction from the external field applied in the j-th direction.
Differential susceptibility
In ferromagnetic crystals, the relationship between M and H is not linear. To accommodate this, a more general definition of differential susceptibility is used
where
is a tensor derived from partial derivatives of components of M with respect to components of H. When the coercivity of the material parallel to an applied field is the smaller of the two, the differential susceptibility is a function of the applied field and self interactions, such as the magnetic anisotropy. When the material is not saturated, the effect will be nonlinear and dependent upon the domain wall configuration of the material.
Susceptibility in the frequency domain
When the magnetic susceptibility is measured in response to an AC magnetic field (i.e. a magnetic field that varies sinusoidally), this is called AC susceptibility. AC susceptibility (and the closely-related "AC permeability") are complex quantities, and various phenomena (such as resonances) can be seen in AC susceptibility that cannot in constant-field (DC) susceptibility. In particular, when an ac-field is applied perpendicular to the detection direction (called the "transverse susceptibility" regardless of the frequency), the effect has a peak at the ferromagnetic resonance frequency of the material with a given static applied field. Currently, this effect is called the microwave permeability or network ferromagnetic resonance in the literature. These results are sensitive to the domain wall configuration of the material and eddy currents.
In terms of ferromagnetic resonance, the effect of an ac-field applied along the direction of the magnetization is called parallel pumping.
For a tutorial with more information on AC susceptibility measurements, see here (external link).
Examples
| Material | Temperature | Pressure | χmol (molar susc.) | χmass (mass susc.) | χv (volume susc.) | M (molar mass) | ρ (density) | |||
|---|---|---|---|---|---|---|---|---|---|---|
| Units | (°C) | (atm) | SI (m3·mol−1) |
cgs (cm3·mol−1) |
SI (m3·kg−1) |
cgs (cm3·g−1) |
SI |
cgs (emu) |
(10-3 kg/mol) or (g/mol) |
(103 kg/m3) or (g/cm3) |
| vacuum | Any | 0 | 0 | 0 | 0 | 0 | 0 | 0 | – | 0 |
| water [10] | 20 | 1 | −1.631×10−10 | −1.298×10−5 | −9.051×10−9 | −7.203×10−7 | −9.035×10−6 | −7.190×10−7 | 18.015 | 0.9982 |
| bismuth [11] | 20 | 1 | −3.55×10−9 | −2.82×10−4 | −1.70×10−8 | −1.35×10−6 | −1.66×10−4 | −1.32×10−5 | 208.98 | 9.78 |
| Diamond [12] | r.t. | 1 | −6.9×10−11 | −5.5×10−6 | −5.8×10−9 | −4.6×10−7 | −2.0×10−5 | −1.6×10−6 | 12.01 | 3.513 |
| He [13] | 20 | 1 | −2.38×10−11 | −1.89×10−6 | −5.93×10−9 | −4.72×10−7 | −9.85×10−10 | −7.84×10−11 | 4.0026 | 0.000166 |
| Xe [13] | 20 | 1 | −5.71×10−10 | −4.54×10−5 | −4.35×10-9 | −3.46×10−7 | −2.37×10−8 | −1.89×10−9 | 131.29 | 0.00546 |
| O2 [13] | 20 | 0.209 | 4.3×10−8 | 3.42×10−3 | 1.34×10−6 | 1.07×10−4 | 3.73×10−7 | 2.97×10−8 | 31.99 | 0.000278 |
| N2 [13] | 20 | 0.781 | −1.56×10−10 | −1.24×10−5 | −5.56×10−9 | −4.43×10−7 | −5.06×10−9 | −4.03×10−10 | 28.01 | 0.000910 |
| Al | 1 | 2.2×10−10 | 1.7×10−5 | 7.9×10−9 | 6.3×10−7 | 2.2×10−5 | 1.75×10−6 | 26.98 | 2.70 | |
| Ag [14] | 961 | 1 | −2.31×10−5 | −1.84×10−6 | 107.87 | |||||
Sources of confusion in published data
There are tables of magnetic susceptibility values published on-line that seem to have been uploaded from a substandard source,[15] which itself has probably borrowed heavily from the CRC Handbook of Chemistry and Physics. Some of the data (e.g. for Al, Bi, and diamond) are apparently in cgs Molar Susceptibility units, whereas that for water is in Mass Susceptibility units (see discussion above). The susceptibility table in the CRC Handbook is known to suffer from similar errors, and even to contain sign errors. Effort should be made to trace the data in such tables to the original sources, and to double-check the proper usage of units. Use them at your own risk!
See also
- Maxwell's equations
- Magnetic flux density
- Electric susceptibility
- Curie constant
- Magnetometer
- Paleomagnetism
- Magnetism
- Iron
- Permeability (electromagnetism)
- magnetic constant
References and notes
- ^ Magnetic properties of materials
- ^ a b Bennett, L. H.; Page, C. H.; and Swartzendruber, L. J. (1978). "Comments on units in magnetism". Journal of Research of the National Bureau of Standards 83 (1): 9-12. NIST, USA.
- ^ L. N. Mulay (1972). in A. Weissberger and B. W. Rossiter: Techniques of Chemistry 4. Wiley-Interscience: New York, p. 431.
- ^ Magway Magnetic Susceptibility Balances
- ^ J. R. Zimmerman, and M. R. Foster (1957). "Standardization of NMR high resolution spectra". J. Phys. Chem. 61: 282-289. doi:.
- ^ Robert Engel, Donald Halpern, and Susan Bienenfeld (1973). "Determination of magnetic moments in solution by nuclear magnetic resonance spectrometry". Anal. Chem. 45: 367-369. doi:.
- ^ P. W. Kuchel, B. E. Chapman, W. A. Bubb, P. E. Hansen, C. J. Durrant, and M. P. Hertzberg (2003). "Magnetic susceptibility: solutions, emulsions, and cells". Concepts Magn. Reson. A 18: 56-71. doi:.
- ^ K. Frei and H. J. Bernstein (1962). "Method for determining magnetic susceptibilities by NMR". J. Chem. Phys. 37: 1891-1892. doi:.
- ^ R. E. Hoffman (2003). "Variations on the chemical shift of TMS". J. Magn. Reson. 163: 325-331. doi:.
- ^ G. P. Arrighini, M. Maestro, and R. Moccia (1968). "Magnetic Properties of Polyatomic Molecules: Magnetic Susceptibility of H2O, NH3, CH4, H2O2". J. Chem. Phys. 49: 882-889. doi:.
- ^ S. Otake, M. Momiuchi and N. Matsuno (1980). "Temperature Dependence of the Magnetic Susceptibility of Bismuth". J. Phys. Soc. Jap. 49 (5): 1824-1828. doi:. The tensor needs to be averaged over all orientations:
. - ^ J. Heremans, C. H. Olk and D. T. Morelli (1994). "Magnetic Susceptibility of Carbon Structures". Phys. Rev. B 49 (21): 15122-15125. doi:.
- ^ a b c d R. E. Glick (1961). "On the Diamagnetic Susceptibility of Gases". J. Phys. Chem. 65 (9): 1552-1555. doi:.
- ^ R. Dupree and C. J. Ford (1973). "Magnetic susceptibility of the noble metals around their melting points". Phys. Rev. B 8 (4): 1780–1782. doi:.
- ^ Magnetic Properties Susceptibilities Chart from READE
Wikipedia content modification information:
- This page was last modified on 8 October 2008, at 21:14.
Wikipedia Authorship and Review
Wikipedia content provided here is not reviewed directly by MedLibrary.org. Wikipedia content is authored by an open community of volunteers and is not produced by or in any way affiliated with MedLibrary.org.
Wikipedia Usage Guidelines
This article is licensed under the GNU Free Documentation License. It uses material from the Wikipedia article on "Magnetic susceptibility".
The URL for this specific entry is:
All Wikipedia text is available under the terms of the GNU Free Documentation License. (See Copyrights for details). Wikipedia® is a registered trademark of the Wikimedia Foundation, Inc.